Introduction to Electrical Steel: Silicon Content, Grades and Magnetic Properties

Nov 22, 2023

Leave a message

What Electrical Steel Is

Electrical steel, also called silicon electrical steel, lamination steel or transformer steel, is a flat-rolled iron-silicon alloy developed for magnetic duty rather than for structural duty. When a magnetic core is magnetised and demagnetised it absorbs energy and heats up; electrical steel exists to reduce that loss and to keep the magnetising current as low as possible. The two properties that matter are a small hysteresis loop area and high magnetic permeability.

Silicon Content and Why It Is Capped Near 3.2 %

The alloy may contain from essentially zero silicon up to 6.5 % silicon. Commercial production grades normally stop at about 3.2 % silicon, because higher silicon contents raise resistivity and lower core loss but make the strip brittle and difficult to cold roll. Manganese and aluminium may be added in amounts up to about 0.5 % to control inclusions and to improve resistivity. The material is supplied as cold-rolled strip, usually less than 2 mm thick, in coil form; when the strips are stacked to build a core the assembly is called a lamination stack. Typical density for 3 % silicon grades is about 7.6 to 7.65 g/cm3, which is used to convert measured mass into the stacking factor of a core.

Loss Separation: Hysteresis, Eddy Current and Interlaminar Losses

Classical magnetic theory treats total core loss as the sum of three parts. Hysteresis loss depends on the alloy and the heat treatment and scales with the area of the B-H loop. Eddy current loss is induced inside each individual lamination and falls as thickness squared, which is why thin grades are used at high frequency. Interlaminar loss appears when adjacent laminations are not adequately insulated from each other and short-circuit paths develop across the stack; the insulating coating applied by the mill is what prevents it. Because loss is the graded property in nearly all purchasing documents, it is also the property that determines the grade name.

Grain-Oriented and Non-Oriented Electrical Steel

Family Grain structure Typical thickness Main application
Grain-oriented (CRGO) Goss texture, easy magnetisation along rolling direction 0.23 mm, 0.27 mm, 0.30 mm Power and distribution transformer cores
Non-oriented (CRNGO) Random grain orientation in the strip plane 0.35 mm, 0.50 mm, 0.65 mm Motors, generators, reactors, small transformers

Grain-oriented strip is used with the flux path aligned to the rolling direction, because magnetic induction is highest in that direction and magnetostriction, which is the main source of transformer audible noise, is lowest. Non-oriented strip is used where the flux path rotates in the plane of the sheet, as it does in the stator and rotor of a motor, so a uniform property in all directions is more valuable than a high value in one.

AISI Grade Designations Still Used in Procurement

To unify specification, production and procurement, electrical steel was historically graded by core loss and given an AISI model number. Non-oriented designations in common use include M-15, M-19, M-22, M-27, M-36, M-43, M-45 and M-47; oriented designations include M-2, M-3, M-4 and M-6. These designations remain widely quoted in enquiry documents even where the governing specification is now a national or international standard, so a purchase order should always pair the grade name with the standard that defines the permissible core loss and induction.

Standards and Test Methods

Fully processed grain-oriented strip is normally ordered to ASTM A876/A876M or EN 10107; fully processed non-oriented strip to ASTM A677/A677M or EN 10106. Magnetic properties are verified by the Epstein frame method described in ASTM A343/A343M and IEC 60404-2, or on ring and toroidal specimens using IEC 60404-6 and ASTM A927/A927M. Because the measured loss depends on the test method, the specification should always name both the grade and the test standard.

Supply Forms, Slitting and Inventory

Electrical steel is supplied as wide coil; the buyer slits to the width that suits the punching or cutting line, which reduces the number and variety of coil widths that must be held in inventory. Because the magnetic properties are direction-dependent in grain-oriented grades, slitting and stacking must preserve the relation between the rolling direction and the intended flux path. Cutting a lamination with the flux path at 90 degrees to the rolling direction loses most of the benefit of the orientation.

Frequently Asked Questions

Q: Why does commercial electrical steel stop at about 3.2 % silicon?
A: Higher silicon lowers core loss but embrittles the strip. Beyond roughly 3.2 % the material can no longer be cold rolled economically into thin strip, so commercial grades stay below that figure even though the alloy system extends to 6.5 %.

Q: Is electrical steel the same as silicon steel?
A: In practice yes. Electrical steel, lamination steel, transformer steel and silicon steel all describe flat-rolled iron-silicon alloys produced for magnetic cores.

Q: Why are transformer cores laminated rather than solid?
A: A solid core would carry large eddy currents. Laminating the core and insulating the sheets from each other breaks those paths and reduces eddy current loss.

Q: Which standard defines grain-oriented electrical steel?
A: ASTM A876/A876M and EN 10107 for fully processed grain-oriented strip, with magnetic properties verified by ASTM A343/A343M or IEC 60404-2.

Q: What does the AISI M designation on a grade mean?
A: It is a legacy designation developed because electrical steel is graded by core loss. The designation is still quoted in enquiries, but the permissible loss and induction values must be taken from the current standard named in the order.

Q: Does thickness affect core loss?
A: Yes. Eddy current loss varies with the square of strip thickness, which is why 0.23 mm and 0.27 mm grades are chosen for transformer cores and 0.50 mm and thicker grades for motor cores.

Send Inquiry