Silicon Steel: Composition, Classification, Properties and Typical Grades
Oct 20, 2025
Leave a message
What Silicon Steel Is and Why It Dominates Magnetic Circuits
Silicon steel, also called electrical steel, is an iron-silicon alloy steel. The silicon addition gives the material soft magnetic behaviour and raises its electrical resistivity, which is why the grade is used as the magnetic material in motors, transformers, electrical appliances and electrical instruments. More electrical energy is converted and distributed through silicon steel than through any other soft magnetic material.
Because the material is produced as thin, flat strip, it can be punched, sheared and stacked into laminated cores with insulated surfaces, and the resulting stack carries the working flux of the machine at a loss level that no plain carbon steel can match.
Composition and Classification: GO, NGO, RGO and HGO
Silicon steel is generally a low-carbon steel with a silicon content of 0.5 % to 4.5 %. It is divided into two categories: grain-oriented, abbreviated GO, and non-oriented, abbreviated NGO, silicon steel. Grain-oriented silicon steel is further classified into regular grain-oriented, RGO, and high-magnetic-permeability grain-oriented, HGO, steel. The oriented family is produced by cold rolling followed by a controlled secondary recrystallisation anneal that aligns the easy magnetisation axis with the rolling direction, so its properties are strongly directional. The non-oriented family has a more random grain orientation and therefore delivers more uniform properties in every direction of the sheet, which suits rotating machines. Hot-rolled silicon steel production has been phased out, and the grades currently supplied are all cold-rolled.
Magnetic and Mechanical Characteristics
Silicon steel has high magnetic permeability, low coercivity and high electrical resistivity, and this combination results in low hysteresis loss and low eddy-current loss at the usual operating inductions. The remaining requirements come from the way the strip is used in manufacturing:
Ductility: the sheet must tolerate the punching and shearing operations used in the production of cores and stator laminations without cracked edges.
Low harmful impurities: carbon, sulphur, nitrogen and oxide inclusions must be kept as low as possible, because they depress magnetic induction and raise hysteresis loss.
Shape and surface: a flat plate shape and good surface quality are needed for tight stacking factors and for stable lamination insulation.
Resistivity: raising resistivity with silicon is the fundamental reason why eddy-current loss in laminated cores stays low.
Typical Grade Families and Loss Data
The grade designation used in the domestic standard system carries two pieces of information: the first two digits give the nominal thickness in hundredths of a millimetre, so 23 means 0.23 mm, and the final digits give the maximum core loss in hundredths of a watt per kilogram, so 110 means 1.10 W/kg. The table below lists representative grades with their maximum core loss measured at 1.7 T and 50 Hz, their lamination factor, and the minimum magnetic induction measured at a field strength of 800 A/m.
| Family | Grade | Strip width (mm) | Max core loss at 1.7 T, 50 Hz (W/kg) | Lamination factor (%) | Min induction at 800 A/m (T) |
|---|---|---|---|---|---|
| Common oriented type | 23Q110 | 35-1200 | 1.10 | 97.2 | 1.82 |
| Common oriented type | 23Q120 | 35-1200 | 1.20 | 97.2 | 1.82 |
| Common oriented type | 27Q120 | 35-1200 | 1.20 | 97.5 | 1.82 |
| Common oriented type | 30G120 | 35-1200 | 1.20 | 98.0 | 1.82 |
| High-induction type | B20P085 | 35-1200 | 0.85 | 97.0 | 1.86 |
| High-induction type | B23P095 | 35-1200 | 0.95 | 97.2 | 1.88 |
| High-induction type | B27P095 | 35-1200 | 0.95 | 97.5 | 1.89 |
| High-induction type | 27QG100 | 35-1200 | 1.00 | 97.5 | 1.89 |
| Domain-refined type | B20R070 | 35-1200 | 0.70 | 97.0 | 1.86 |
| Domain-refined type | B23R085 | 35-1200 | 0.85 | 97.2 | 1.88 |
| Domain-refined type | B27RK085 | 35-1200 | 0.85 | 97.5 | 1.89 |
The high-induction family reaches 1.86 T to 1.89 T at 800 A/m and therefore allows a smaller core for the same power rating, while the domain-refined family, whose surface is treated with a fine laser scribing pattern, lowers core loss further to 0.70 W/kg and is used where no-load loss dominates the total loss. Thickness in the families listed ranges from 0.20 mm to 0.30 mm, and the strip is supplied in widths from 35 mm to 1200 mm so that both large wound cores and narrow punched laminations can be produced from the same coil.
Applications from Small Relays to Large Transformers
Silicon steel is the most widely used soft magnetic material of all. Application quantities range from a few ounces in small relays and pulse transformers to several tons in generators, motors and transformers. Grain-oriented steel is used in large quantities, mainly in power and distribution transformers, where the flux path follows the rolling direction and the low hysteresis loss of the oriented grain structure is fully exploited. Non-oriented steel is used in areas requiring low-cost, low-loss material, especially in rotating equipment such as motors and generators, and in small transformers, reactors and instrument parts where the flux rotates rather than following one fixed direction. Electrical instruments, voltage stabilisers, welding equipment and magnetic amplifiers form additional volume applications.
Frequently Asked Questions
Q: What silicon content is used in electrical steel?
Silicon steel normally contains 0.5 % to 4.5 % silicon balanced by iron and a very low carbon level; the exact figure is fixed by the grade and by the required balance between resistivity and ductility.
Q: What is the difference between grain-oriented and non-oriented silicon steel?
Grain-oriented steel has a controlled grain orientation aligned with the rolling direction and is used in transformers, while non-oriented steel has a more random orientation and gives uniform properties in all directions for motors and generators.
Q: What do the numbers in a grade such as 23Q110 mean?
The first two digits give the nominal thickness in hundredths of a millimetre, so 0.23 mm, and the last digits give the maximum core loss of 1.10 W/kg measured at 1.7 T and 50 Hz.
Q: Why is grain-oriented steel preferred for distribution transformers?
Its easy magnetisation axis lies along the rolling direction, so a wound or mitred core that follows that direction needs a lower exciting current and produces lower no-load loss.
Q: Is hot-rolled silicon steel still available?
Hot-rolled silicon steel production has been phased out and the material currently supplied is cold-rolled, either grain-oriented or non-oriented, depending on the application.
Q: What thickness and width are available?
The grades listed above are supplied in thickness from 0.20 mm to 0.30 mm and in strip widths from 35 mm to 1200 mm, which covers both narrow laminations and large wound cores.