How Chinese and Japanese Silicon Steel Sheet Grades Are Expressed
Oct 27, 2023
Leave a message
Silicon steel sheet is ordered by a grade code, and that code is effectively a compressed datasheet. It states whether the steel is hot rolled or cold rolled, whether it is grain oriented or non-oriented, how thick the sheet is and how much core loss the buyer should expect. China and Japan use different letters for the same information, which causes avoidable confusion whenever quotations from the two systems are compared side by side.
The Chinese Designation System
Chinese grades begin with a letter group that identifies the product family, followed by the guaranteed iron loss value multiplied by 100, and finally the nominal thickness in millimetres multiplied by 100. Current GB/T 2521 notation places the thickness factor first and uses a single letter for the product family, while the older two-letter form still appears on many drawings and enquiry sheets.
| Letter group | Product family | Comments |
|---|---|---|
| DW | Cold-rolled non-oriented silicon steel strip and sheet | Older form, now written as W |
| DQ | Cold-rolled grain-oriented silicon steel strip and sheet | Older form, now written as Q |
| DR | Hot-rolled silicon steel plate | Split by silicon content |
| JDR | Hot-rolled silicon steel sheet for household appliances | Appliance-specific grades |
| W | Non-oriented cold-rolled steel in current notation | Thickness factor written first |
| Q | Oriented cold-rolled steel in current notation | Thickness factor written first |
Reading a Non-Oriented Grade: DW470-50 and 50W470
DW470-50 was written in the older style. DW identifies cold-rolled non-oriented strip, 470 is the specific iron loss value multiplied by 100, and 50 is the nominal thickness in millimetres multiplied by 100. The loss value is defined at 50 Hz with a sinusoidal induction peak of 1.5 T. The grade therefore describes material with a loss of 4.70 W/kg at 1.5 T and 50 Hz in sheet 0.50 mm thick. Under current notation the same product is written 50W470: the thickness factor comes first, W replaces the two-letter prefix, and the loss figure is unchanged. A 0.35 mm version of the same loss class becomes 35W470.
Reading Oriented and Hot-Rolled Grades
Oriented grades are quoted at a higher induction, normally 1.7 T at 50 Hz. DQ133-30 denotes cold-rolled grain-oriented strip with a loss of 1.33 W/kg and a thickness of 0.30 mm, and current notation expresses the same material as 30Q133. Where a G is added after the loss value in the older form, it marks a grade with high magnetic induction, so the induction level must be checked against the mill certificate rather than assumed from the code alone.
Hot-rolled silicon steel plate uses the DR prefix and is divided by silicon content into low-silicon grades with silicon up to 2.8 percent and high-silicon grades above 2.8 percent. The code follows the same logic, DR plus the loss value multiplied by 100 plus the thickness multiplied by 100, so DR510-50 describes hot-rolled plate with a loss of 5.10 W/kg and a thickness of 0.50 mm. Household appliance grades add the J prefix in front of DR, for example JDR540-50.
The Japanese Designation System
Japanese grades follow a different order. Non-oriented strip is written as nominal thickness multiplied by 100, then the letter A, then the guaranteed loss value multiplied by 100 at 50 Hz and 1.5 T. The grade 50A470 therefore means non-oriented strip 0.50 mm thick with a guaranteed loss value no greater than 4.70 W/kg. Oriented strip uses the letter G for ordinary material and the letter P for high-orientation material, again preceded by the thickness factor and followed by the loss value at 1.7 T and 50 Hz. Thus 30G130 is oriented strip 0.30 mm thick with a guaranteed loss of 1.30 W/kg, and 30P120 is a high-orientation grade of the same thickness with a guaranteed loss of 1.20 W/kg. Grade definitions come from national standards, GB/T 2521 for cold-rolled electrical steel in China and the JIS C 2550 series in Japan, with IEC 60404-8-7 covering grain-oriented and IEC 60404-8-4 covering non-oriented material at international level.
Mapping the Two Systems
| Product | Chinese designation | Japanese designation | Loss reference condition |
|---|---|---|---|
| Non-oriented, 0.50 mm, 4.70 W/kg | 50W470 (older: DW470-50) | 50A470 | 1.5 T at 50 Hz |
| Non-oriented, 0.35 mm, 4.70 W/kg | 35W470 | 35A470 | 1.5 T at 50 Hz |
| Oriented, 0.30 mm, 1.33 W/kg | 30Q133 | 30G130 class | 1.7 T at 50 Hz |
| High-orientation, 0.30 mm, low loss | 30Q120 | 30P120 | 1.7 T at 50 Hz |
The mapping is indicative rather than exact. The two systems quote guaranteed values under the same reference induction and frequency, but thickness tolerances, permissible loss tolerances and the permissible induction at a given field strength differ between standards, and a supplier may also state typical rather than guaranteed figures. Buyers should always compare the mill test certificates rather than the grade codes alone.
Practical Points When Comparing Offers
Check the thickness factor first: 35 in the code means 0.35 mm, not 0.35 cm or a loss value.
Confirm which induction and frequency the loss guarantee refers to, since oriented grades are quoted at 1.7 T and non-oriented at 1.5 T.
Verify whether the quoted loss is a guaranteed maximum or a typical value, because the two differ by a tolerance band.
Confirm how many digits follow the letter; converting between the old and new Chinese forms requires swapping the position of the thickness factor, not changing its value.
Ask for the grade as stated in the governing standard when an order is placed, so that the mill cannot substitute an alternative notation.
Frequently Asked Questions
Q: What does the number after the letter W mean in 50W470?
It is the specific iron loss value multiplied by 100, measured at 50 Hz with a sinusoidal induction peak of 1.5 T, so 470 corresponds to 4.70 W/kg.
Q: How do I convert DW470-50 into the current Chinese notation?
Move the thickness factor to the front and replace DW with W, which gives 50W470. The numerical value of the thickness factor and the loss value stay the same.
Q: What is the difference between the letters G and P in Japanese oriented grades?
G marks ordinary grain-oriented material and P marks high-orientation material with lower loss and higher permeability. Both are prefixed by the thickness factor and followed by the loss value.
Q: Why are oriented grades quoted at 1.7 T instead of 1.5 T?
Because oriented steel is designed for the higher working induction found in transformer cores, the loss guarantee is defined at 1.7 T and 50 Hz rather than at 1.5 T.
Q: What distinguishes low-silicon from high-silicon hot-rolled plate?
The dividing line is a silicon content of 2.8 percent. Grades at or below that level are low-silicon, and grades above it are high-silicon, with corresponding differences in resistivity and loss.
Q: Can an equivalent grade always be substituted across systems?
Not automatically. Loss and thickness classes may align, but tolerances and guaranteed conditions differ between standards, so the mill certificate must be compared before any substitution.