What an Amorphous C-Type Core Is
An amorphous C-type core is assembled from iron-based amorphous alloy ribbon (Fe-Si-B) that is wound into a rectangular block and then opened by a single diamond cut, producing two C-shaped halves with flat mating faces. The ribbon is made by melt spinning, which quenches liquid alloy at roughly 106 K/s; at that cooling rate the alloy never develops a long-range crystal lattice, so there are no grain boundaries to pin domain walls and no crystallographic easy axis to oppose magnetisation. The material therefore behaves as a very soft magnet: high permeability, low coercivity, and a hysteresis loss that stays low as frequency rises.
For a designer the practical difference is magnetic path thickness. Amorphous ribbon is typically 0.020-0.030 mm thick, far thinner than any laminated silicon steel sheet, which keeps the eddy-current component of loss small at the switching frequencies used in modern converters. Typical saturation induction of Fe-based amorphous ribbon is about 1.56 T, against roughly 1.9 T for grain-oriented silicon steel and 0.4-0.5 T for MnZn ferrite, so a cut core sits between laminated steel and ferrite for a given energy storage requirement.
Design Features of the Cut-Core Format
No crystalline structure: the absence of grain boundaries removes the domain-wall pinning that dominates loss in crystalline soft magnetic materials.
Low core loss: thin ribbon plus a disordered lattice suppress both the hysteresis and the eddy-current components.
High saturation flux density: about 1.56 T means fewer turns and a smaller winding window for the same stored energy.
High permeability: higher inductance per turn, which shortens the winding and reduces copper loss.
Rectangular window: simple bobbin assembly, and the cut gap can be shimmed or ground to set inductance precisely.
Temperature stability: saturation induction and permeability change little over the normal operating band, unlike ferrite, whose saturation induction falls sharply near its Curie point.
Standard C-Core Dimension Series
The table below lists a representative build series in millimetres. Dimensions a and d carry the tightest tolerance because they control the mating faces and therefore the effective gap; e and f are the outer envelope and are held more loosely.
| Build a (mm) | b (mm) | c (mm) | d (mm) | e (mm) | f (mm) |
|---|---|---|---|---|---|
| 9 ± 0.5 | 10 | 32.8 | 15 ± 0.5 | 28 ± 1 | 50.8 ± 1.25 |
| 10 ± 0.5 | 11 | 33 | 20 ± 0.5 | 31 ± 1 | 53 ± 2 |
| 11 ± 0.5 | 13 | 30 | 20 ± 0.5 | 35 ± 1 | 52 ± 2 |
| 11 ± 0.5 | 13 | 40 | 20 ± 0.5 | 35 ± 1 | 62 ± 2 |
| 11 ± 0.5 | 13 | 40 | 25 ± 0.5 | 35 ± 1 | 62 ± 2 |
Larger builds are normally made to drawing rather than to a catalogue series, because the winding window is usually fixed by the copper and the cooling path is fixed by the enclosure.
Matching the Core to the Circuit
Selection starts from the flux swing, the frequency and the DC bias, not from the core size. A cut core with a defined gap is the standard choice wherever the inductor carries a large DC component, because the gap stores energy in the air path and keeps the core away from saturation.
Solar and energy-storage inverter filters, 8-20 kHz: the core operates with a large ripple and moderate DC bias; a small to medium build with a shimmed gap gives predictable inductance and moderate loss.
Power factor correction chokes, 20-60 kHz: loss density dominates, so a thinner, higher-permeability build is preferred and the gap is set to keep peak flux below saturation at the worst-case line condition.
Medium-frequency transformers, 1-20 kHz: no intentional gap; the two halves are bonded or clamped closed, and the design trade is copper loss against core loss.
Energy-storage and differential-mode chokes: inductance is the controlling parameter, so the design is driven by the effective permeability after gapping.
Gapping, Winding and Assembly Practice
Effective permeability after a gap is set by the ratio of the magnetic path length to the gap length, so a very small non-magnetic shim produces a large drop in inductance. Production practice is to gap on the bench with the coil in place and to measure inductance and DC-bias saturation current on every unit, because the mating-face finish is the dominant variable. Two further points matter: the halves must be clamped with consistent pressure, since a loose clamp adds an uncontrolled gap; and the winding should be distributed around the window rather than bunched, to limit leakage flux and the resulting eddy currents in the copper.
How Magnetic Properties Are Verified
Amorphous strip is specified against GB/T 19345.1-2017, which covers Fe-based amorphous soft magnetic alloy strip, its dimensions, surface condition and property classes. Because a cut core is a wound structure rather than stamped sheet, the applicable measurement methods are IEC 60404-6, which defines measurement of the magnetic properties of magnetically soft metallic and powder materials at frequencies from 20 Hz to 100 kHz using ring specimens, and ASTM A927/A927M, the voltmeter-ammeter-wattmeter method for toroidal core specimens. A supplier certificate should always state flux density, frequency and temperature alongside the loss figure, because loss numbers taken at different test points cannot be compared directly.
Frequently Asked Questions
Q: What is the saturation flux density of an amorphous C-type core?
A: Standard Fe-Si-B amorphous ribbon saturates at approximately 1.56 T, which is lower than grain-oriented silicon steel at about 1.9 T but much higher than MnZn ferrite at 0.4-0.5 T
Q: Can this core be used at 50 Hz?
A: Yes, but at power frequency the loss advantage over laminated silicon steel narrows and a gapped cut core is usually chosen for its DC-bias tolerance rather than for its loss
Q: How is inductance adjusted in production?
A: A non-magnetic shim of known thickness is inserted between the mating faces; inductance falls approximately in proportion to the added gap length, and the final value is verified on each wound unit
Q: What is the maximum operating temperature?
A: The ribbon keeps its soft magnetic properties up to well above 450 °C, but in practice the class 130-155 °C limit of the impregnating resin, tape and bobbin governs the design
Q: Is a coating required on the cut faces?
A: The ribbon carries a thin insulating surface layer, and cut or ground faces are normally coated with a thin epoxy to prevent edge shorts between turns of the core
Q: How does a cut core compare with a powdered iron core?
A: Above about 10 kHz a cut core generally offers lower loss for the same inductance, while powdered iron tolerates softer saturation; the choice is made on loss budget and bias requirement